[DeTomaso] Brazing

David Fisher fisher95020 at gmail.com
Thu Oct 25 11:59:51 EDT 2012


Ah how I love the collective wisdom of the mailing list.   Lot's of good
advice.

I probably should have mentioned that I am using Oxy-Acetylene with flux
coated rods and I do get a popping and sizzling sound when things get
porous.

It seems that Larry has probably diagnosed it correctly..   I am probably
boiling the filler and evaporating one of the filler metals.

Thanks Guys!



On Thu, Oct 25, 2012 at 6:23 AM, Larry - Ohio Time Corp <
larry at ohiotimecorp.com> wrote:

> David,
>
> If every thing is dry and clean. The flux is good, as others have said.
> Make
> sure you are not over heating the braze metal. It will "boil" (out gas??)
> and look like this.
>
> Larry - Cleveland
>
> -----Original Message-----
> From: detomaso-bounces at realbig.com [mailto:detomaso-bounces at realbig.com]
> On
> Behalf Of David Fisher
> Sent: Thursday, October 25, 2012 3:46 AM
> To: DeTomaso Forum
> Subject: [DeTomaso] Brazing
>
> Any of you craftsman  out there that can tell me why my brazing is
> sometimes porous?  I am getting tiny little holes in the brass.
>
> Too much heat, oxygen, not enough, etc?   Anyone found any good online
> resources for this?
>
> I know it's a bit of a lost art, but I find myself doing it occasionally on
> my Jaguar as that was the factory practice.
>
> Pic attached
>
> http://www.poca.com/index.php/gallery/?g2_itemId=38384
>
>
> Thanks
>
> David
> _______________________________________________
>
> Detomaso Forum Managed by POCA
>
> Archive Search Engine Now Available at http://www.realbig.com/detomaso/
>
> DeTomaso mailing list
> DeTomaso at realbig.com
> http://realbig.com/cgi-bin/mailman/listinfo/detomaso
>
>



More information about the DeTomaso mailing list